تفاصيل المنتج
مكان المنشأ: الصين
اسم العلامة التجارية: Tankii
إصدار الشهادات: ISO 9001
رقم الموديل: 1CR13AL4
شروط الدفع والشحن
الحد الأدنى لكمية: 5 كجم
الأسعار: قابل للتفاوض
تفاصيل التغليف: التخزين المؤقت
وقت التسليم: 10-15days
شروط الدفع: تي / تي، خطاب الاعتماد
القدرة على العرض: 500 طن / سنة
FeCrAl Allloy Strip (1Cr13Al14/CrAl14/FeCrAl134)
Nominal Analysis
14.00 Cr, 4.00 Al, Bal. Fe
Max contineous working temperature: 950º C.
Melting Temperature: 1450º C
Electrical Resistivity: 1.25 ohm mm2/m
Has been used extensively as heating elements in industrial furnaces and electrical kilns.
Has less hot strength than Tophet alloys but much higher melting point.
Shanghai TANKII ALLOY MATERIAL CO., LTD.
ALCHROME ALLOY PRODUCER IN CHINA
| Chemical Composition and Main Property of Fe-Cr-Al Resistance Alloy |
||||||||
| Properties Grade |
1Cr13Al4 |
0Cr25Al5 |
0Cr21Al6 |
0Cr23Al5 |
0Cr21Al4 |
0Cr21Al6Nb |
0Cr27Al7Mo2 |
|
| Main Chemical Composition (%) |
Cr |
12.0-15.0 |
23.0-26.0 |
19.0-22.0 |
22.5-24.5 |
18.0-21.0 |
21.0-23.0 |
26.5-27.8 |
| Al |
4.0-6.0 |
4.5-6.5 |
5.0-7.0 |
4.2-5.0 |
3.0-4.2 |
5.0-7.0 |
6.0-7.0 |
|
| Re |
opportune |
opportune |
opportune |
opportune |
opportune |
opportune |
opportune |
|
| Fe |
Bal. |
Bal. |
Bal. |
Bal. |
Bal. |
Bal. |
Bal. |
|
| Nb0.5 |
Mo1.8-2.2 |
|||||||
| Max Continuous Service Temperature(oC) |
950 |
1250 |
1250 |
1250 |
1100 |
1350 |
1400 |
|
| Resisivity 20oC (Ωmm2/m) |
1.25 ±0.08 |
1.42 ±0.06 |
1.42 ±0.07 |
1.35 ±0.07 |
1.23 ±0.07 |
1.45 ±0.07 |
1.53 ±0.07 |
|
| Density(g/cm3) |
7.4 |
7.1 |
7.16 |
7.25 |
7.35 |
7.1 |
7.1 |
|
| Thermal Conductivity |
52.7 |
46.1 |
63.2 |
60.2 |
46.9 |
46.1 |
45.2 |
|
| (KJ/m@h@oC) |
||||||||
| Coefficient of Thermal Expansion(α×10-6/oC) |
15.4 |
16 |
14.7 |
15 |
13.5 |
16 |
16 |
|
| Approximate Melting Point( oC) |
1450 |
1500 |
1500 |
1500 |
1500 |
1510 |
1520 |
|
| Tensile Strength(N/mm2) |
580-680 |
630-780 |
630-780 |
630-780 |
600-700 |
650-800 |
680-830 |
|
| Elongation(%) |
>16 |
>12 |
>12 |
>12 |
>12 |
>12 |
>10 |
|
| Section Variation |
65-75 |
60-75 |
65-75 |
65-75 |
65-75 |
65-75 |
65-75 |
|
| Shrink Rate (%) |
||||||||
| Repeatedly Bend Frequency(F/R) |
>5 |
>5 |
>5 |
>5 |
>5 |
>5 |
>5 |
|
| Hardness (H.B.) |
200-260 |
200-260 |
200-260 |
200-260 |
200-260 |
200-260 |
200-260 |
|
| Continuous Service Time |
no |
≥80/1300 |
≥80/1300 |
≥80/1300 |
≥80/1250 |
≥50/1350 |
≥50/1350 |
|
| Micrographic Structure |
Ferrite |
Ferrite |
Ferrite |
Ferrite |
Ferrite |
Ferrite |
Ferrite |
|
| Magnetic Property |
Magnetic |
Magnetic |
Magnetic |
Magnetic |
Magnetic |
Magnetic |
Magnetic |
|
![]()
![]()
![]()
![]()
![]()